Created on 11.09

F92 Valve Seat Hardfacing: Inconel 625 and Stellite 6 TIG Welding

Technical Welding Procedure for F92 Valve Seats with Inconel 625 Buttering Layer and Stellite 6 Hardfacing

Process: GTAW / TIG Welding | Equipment: OTC 315 Welding Machine | Application: High-Temperature and High-Pressure Valve Seat Components

1. Project Overview

The valve seat component is manufactured from F92 (ASTM A182 F92 or equivalent Grade 92 material, subject to material certificate verification), a high-temperature martensitic steel commonly used in demanding power generation and steam service applications.
To improve the wear resistance, erosion resistance, and sealing performance of the valve seat, a multilayer weld overlay system is proposed.
The overlay structure consists of:
  1. Base Material:
F92 martensitic heat-resistant steel, previously heat-treated.
  1. Intermediate Buttering Layer:
Inconel 625 nickel-based alloy, applied by GTAW to provide a metallurgical transition between the F92 substrate and the cobalt-based hardfacing.
  1. Top Hardfacing Layer:
Stellite 6 cobalt-based alloy, deposited to provide approximately 3 mm of finished wear-resistant material, subject to the final machining requirements.
The welding operation is performed using an OTC 315 welding machine with the GTAW/TIG process and high-purity argon shielding gas.
The primary technical challenge is preventing cracking caused by thermal gradients, residual welding stresses, hydrogen-assisted cracking, metallurgical incompatibility, and the relatively low ductility of Stellite 6.

2. Recommended Weld Overlay Structure

Proposed multilayer overlay configuration. Actual deposited thicknesses and machining allowances shall be established through procedure qualification.
Layer
Recommended material
Technical purpose
Substrate
ASTM A182 F92 / equivalent
Structural strength and high-temperature performance
Buttering layer
ERNiCrMo-3 / Alloy 625
Metallurgical transition, improved ductility and stress accommodation
Hardfacing
ERCoCr-A / Stellite 6
Wear, erosion and galling resistance
Important: The Inconel 625 layer helps accommodate differences between the F92 substrate and Stellite 6. However, its effectiveness depends on dilution, deposited thickness, weld integrity, and the subsequent thermal treatment.

3. Surface Preparation Before Welding

Before welding, the valve seat shall undergo the following preparation:
  • Verify the F92 material certificate, heat-treatment records, and chemical composition.
  • Confirm the base material condition, including hardness and any previous repair history.
  • Machine the welding surface to remove oxides, defects, contamination, and any damaged material.
  • Provide a smooth transition between the overlay area and the base metal. Avoid sharp corners and abrupt changes in section thickness.
  • Perform PT or MT examination on the prepared substrate surface, as applicable.
  • Clean the welding area using an approved solvent to remove oil, grease, moisture, and other contaminants.
  • Use dedicated stainless steel brushes and clean tools to avoid contamination.
The component should be dry and free from surface defects before preheating.

4. Preheating Procedure

Preheating is essential for controlling the cooling rate of the F92 heat-affected zone and reducing the risk of hydrogen-assisted cracking.
Proposed initial parameters for procedure qualification:
Parameter
Preliminary recommendation
Preheating temperature
200–250°C
Interpass temperature during F92/625 deposition
200–300°C
Heating method
Controlled resistance heating or suitable furnace heating
Temperature monitoring
Calibrated thermocouples
Temperature distribution
Uniform heating across the weld area and adjacent heavy sections
The component shall be heated gradually and uniformly to minimize thermal gradients.
Localized overheating by direct flame should be avoided.
For large valve seat rings, thermocouples should be positioned at several locations to monitor circumferential temperature uniformity.
A preheat of approximately 430°C should not be adopted as a standard starting value without qualification. Although elevated preheat may reduce thermal gradients in some situations, it can also affect transformation behavior, welding metallurgy, and the overall heat-treatment strategy for F92.
The final preheat temperature must be established through a qualified welding procedure.

5. Inconel 625 Intermediate Layer Deposition

The first welding stage involves depositing Inconel 625 onto the F92 substrate using GTAW.

5.1 Welding Consumables and Equipment

Item
Specification
Welding machine
OTC 315, subject to exact model verification
Welding process
GTAW / TIG
Filler metal
AWS A5.14 ERNiCrMo-3
Shielding gas
Argon, typically ≥99.99% purity
Polarity
DCEN
Tungsten electrode
2.4 or 3.2 mm, suitable grade
Welding current
Initial trial range 100–180 A
Arc voltage
Typically 10–15 V, depending on arc length
Shielding gas flow
Typically 10–16 L/min
These are preliminary trial ranges, not qualified production settings. Actual parameters must be adjusted according to wall thickness, welding position, torch configuration, travel speed, and measured heat input.

5.2 Deposition Procedure

The Inconel 625 layer should be deposited using controlled, overlapping weld beads.
A preliminary deposited thickness of approximately 2–3 mm may be considered, depending on dilution and machining requirements.
The welding sequence should be arranged to distribute heat evenly around the circumference of the valve seat.
For ring-shaped components, a balanced or segmented deposition sequence may help reduce distortion and residual stress.
Excessive weaving and prolonged arc dwell should be avoided.
After deposition, the Inconel 625 surface should be inspected and, where necessary, lightly machined to remove surface irregularities before further processing.

6. Intermediate Heat Treatment and F92 Metallurgical Control

This is one of the most critical stages of the entire process.
Although the F92 base material has already undergone its original heat treatment, the subsequent Inconel 625 welding operation creates a new heat-affected zone.
Depending on the welding thermal cycle, this region may contain newly formed, relatively hard martensitic microstructures.
Consequently, the component may require an intermediate post-weld heat treatment before Stellite 6 deposition.

Recommended process strategy

Stage A — F92 + Inconel 625:
After completion of the Inconel 625 buttering layer, conduct the required post-weld heat treatment under an approved F92 procedure.
For Grade 92 materials, tempering/PWHT temperatures commonly fall within a range around 730–780°C, but the exact temperature, holding time, heating/cooling rate, and upper temperature limit must be determined from the applicable construction code, material specification, original heat-treatment condition, and qualified WPS/PQR.
The treatment temperature must not exceed the applicable limit for the specific F92 material condition.
Stage B — Stellite 6:
After completion of the intermediate heat treatment, perform the Stellite 6 hardfacing operation under a separately qualified thermal-control procedure.
This staged approach may reduce the risk of exposing the final Stellite 6 hardfacing layer to a high-temperature F92 PWHT cycle.
However, it does not automatically eliminate the need to evaluate the heat-affected zone created by the final hardfacing operation. The qualification must demonstrate that the final welding thermal cycle does not leave unacceptable hardness, cracking susceptibility, or other metallurgical defects in the F92 substrate.

7. Stellite 6 Hardfacing Procedure

The Stellite 6 layer provides the required sealing surface hardness and resistance to wear, erosion, and metal-to-metal contact damage.

7.1 Welding Parameters

Parameter
Preliminary recommendation
Welding process
GTAW / TIG
Filler metal
AWS A5.21 ERCoCr-A or qualified equivalent
Welding current
Trial range 90–150 A
Polarity
DCEN
Shielding gas
High-purity argon
Gas flow rate
10–16 L/min
Preheat before Stellite deposition
Initial trial 200–300°C
Interpass temperature
Initial trial 200–300°C
Finished Stellite thickness
Approximately 3 mm minimum, if specified
Deposited thickness
Typically 4–5 mm as an initial machining allowance
The exact welding parameters should be established through trial welding and verified by procedure qualification.

7.2 Welding Technique

Stellite 6 should be deposited using controlled stringer beads or limited weaving to reduce excessive heat input and dilution.
The welding operator should maintain a short, stable arc and avoid unnecessary remelting of previously deposited weld metal.
For circular valve seat surfaces, balanced deposition around the circumference is recommended to reduce localized thermal accumulation.
Each weld pass should be visually inspected before proceeding to the next pass.
Crater filling is particularly important because unfilled weld craters may become crack initiation sites.
The final deposited thickness must provide sufficient machining allowance to achieve the specified finished Stellite 6 thickness without exposing the underlying Inconel 625 layer.

8. Crack Prevention and Thermal Stress Control

Cracking in Stellite 6 hardfacing may result from several interacting mechanisms.
Potential cause
Preventive action
Rapid cooling
Controlled preheating and cooling
High thermal gradients
Uniform heating and balanced welding sequence
Excessive residual stress
Low-restraint welding sequence and controlled heat input
Excessive dilution
Optimized bead geometry and multilayer deposition
Hydrogen-assisted cracking in F92 HAZ
Low-hydrogen practice, appropriate preheat and qualified PWHT
Solidification cracking in Stellite 6
Control weld pool geometry, dilution and bead overlap
Sharp geometric transitions
Smooth machining transitions and appropriate edge preparation
Excessive hardfacing thickness
Avoid unnecessary buildup and qualify the final thickness
It is important to distinguish between hydrogen-assisted cracking in the F92 heat-affected zone and solidification or thermal-stress cracking in the Stellite 6 overlay.
These mechanisms require different preventive measures.

9. Post-Weld Hydrogen Control and Cooling

After Stellite 6 deposition, the component should not be subjected to uncontrolled rapid cooling.
A controlled cooling procedure should be used to minimize thermal gradients and residual stresses.
For the F92 substrate, a hydrogen-release hold may be considered as part of the qualified welding procedure. However, a low-temperature hydrogen-release treatment is not equivalent to the required F92 post-weld tempering treatment.
The procedure must clearly distinguish between:
  • Hydrogen-release holding, intended to assist hydrogen diffusion.
  • Controlled cooling, intended to reduce thermal gradients.
  • Post-weld heat treatment, intended to achieve the required metallurgical condition and mechanical properties.
Any proposed hydrogen-release temperature and holding time must be qualified for the actual material thickness, weld sequence, and hydrogen-control requirements.
The component should be protected from drafts and rapid cooling during the controlled cooling stage.

10. Machining After Welding

Following completion of welding, heat treatment, and required inspections, the valve seat shall undergo precision machining.
Based on the supplied workshop photographs, the component appears to be a large annular valve seat with a substantial overlay area. Such components require careful control of concentricity, distortion, and sealing-surface geometry.Lathes for valves machining | CNV, OMG Zanoletti
Hardfaced valve sealing surface
Recommended machining and inspection controls include:
  • Confirm that sufficient Stellite 6 thickness remains after finishing.
  • Verify sealing diameter, concentricity, flatness, and runout against the approved drawing.
  • Use appropriate cutting tools and stable machining parameters for the hard cobalt-based alloy.
  • Avoid excessive cutting heat, chatter, and mechanical loading on the overlay.
  • Perform final surface roughness inspection according to the valve sealing requirements.
For precision sealing surfaces, the final roughness requirement should be specified by the customer drawing and valve design, rather than assigning a universal Ra value.

11. Quality Inspection and Acceptance

The following inspection sequence is recommended:
Inspection stage
Inspection method
Purpose
Before welding
Material verification, hardness, PT/MT
Confirm substrate condition
After Inconel 625 deposition
VT and PT
Identify surface defects
After intermediate PWHT
Hardness testing, PT and additional NDT as required
Verify F92 HAZ condition
After Stellite 6 deposition
VT and PT after appropriate cooling
Detect surface cracks
After final machining
PT, dimensional and roughness inspection
Verify finished overlay
Procedure qualification
Macrosection, hardness traverse, metallography and other specified tests
Validate overlay integrity and metallurgical compatibility
Additional examination such as UT, volumetric testing, or destructive qualification testing may be required depending on the applicable construction code and customer specification.
Acceptance criteria should be established before production. Surface-breaking cracks should not be accepted without a specific, technically justified and code-permitted disposition.

12. Recommended Manufacturing Process Flow

1. F92 material verification and surface preparation
2. Controlled preheating
3. GTAW deposition of Inconel 625 buttering layer
4. Intermediate inspection and qualified F92 PWHT
5. Surface preparation and Stellite 6 preheating
6. GTAW deposition of Stellite 6 hardfacing
7. Controlled cooling and required post-weld treatment
8. Final inspection and precision machining
9. Final PT, dimensional verification and quality release

13. Engineering Recommendations

For F92 valve seats requiring Stellite 6 hardfacing, Win Road Tech. recommends qualifying the Inconel 625 buttering process and Stellite 6 deposition process as an integrated manufacturing procedure.
Particular attention should be given to the following:
  1. Establishing a suitable preheat and interpass temperature range for each welding stage.
  2. Controlling dilution between F92, Inconel 625, and Stellite 6.
  3. Evaluating the need for intermediate PWHT after Inconel 625 deposition.
  4. Preventing excessive residual stress and cracking during Stellite 6 deposition.
  5. Verifying the final F92 heat-affected zone hardness and metallurgical condition.
  6. Maintaining the specified hardfacing thickness after precision machining.
  7. Conducting representative procedure qualification tests before production welding.
Conclusion
The combination of F92 base material, Inconel 625 buttering, and Stellite 6 hardfacing can provide a practical engineering solution for valve components operating under severe temperature, pressure, and wear conditions.
However, successful application depends on properly qualified welding parameters, heat-treatment procedures, dilution control, and final inspection.
The values presented in this document are preliminary engineering recommendations and shall not be treated as an approved Welding Procedure Specification (WPS) until supported by applicable procedure qualification records (PQR) and customer/code approval.

We are committed to excellence in everything we do and look forward to working with you!

QUESTIONS OR CONSULTING

Contact Information

Fill up the form and we’ll get back to you in few hours.

+86 769 82868699

winroad@winroadcn.com

Room 109, Building 3, No. 143 Jinrong Street, Jinju, Dalingshan Town, Dongguan City, Guangdong Province, China. 

Call Us

+86 18302080028

About us

About winroadcn.com

WhatsApp +86 186 7515 7815

E-mail: zoe@winroadcn.com

Customer services

Contact us

Tel
WhatsApp
WeChat